Abstract
A method measuring the thermal conductivity and the interfacial thermal resistance of thermal barrier coatings (TBCs) which consist of metallic bond-coats (BCs) and ceramics top-coats (TCs) on superalloys was newly developed. It was based on the areal heat diffusion time method analysing the heat diffusion across multilayers. The developed method was experimentally verified using the BC and the TBC specimens coated by APS. It was found that there were the interfacial thermal resistance not only between the TC and the BC but also between the BC and the substrate. Furthermore, the thermal conductivities of the BC and the TC obtained from the BC and the TBC specimens by this method considering the interfacial thermal resistance were in good agreement with those measured from the free-standing specimen of each coating. Thus, it was confirmed that the newly developed method is effective to evaluate the thermal conductivity and the interfacial thermal resistance of the TBC.